Toolox 44 – quenched and tempered tool steel
SSAB tool and engineering steel, supplied quenched and tempered at 410 – 475 HBW
Toolox 44 is an SSAB tool and engineering steel supplied quenched and tempered, with a hardness of 410 – 475 HBW (≈ 45 HRC) and high toughness. It arrives ready to machine, with no heat treatment afterward, and keeps its properties up to 590 °C, the minimum factory tempering temperature.
Designations and equivalents
| System | Designation |
|---|---|
| UNS | — (proprietary steel) |
| W.Nr./EN | — (proprietary steel) |
| Trade names | Toolox 44 (SSAB) |
| Others | Same family: Toolox 33, Toolox 40 and Toolox 46 |
Standards by product form
| Form | Standard |
|---|---|
| Plate (6 – 130 mm) | SSAB specification; EN 10029 tolerances (Toolox Thickness Guarantee); EN 10160 ultrasonic testing |
| Forged block (150 – 320 mm) | SSAB specification; EN 10228-3 ultrasonic testing; flatness max. 1 mm/m |
| Round bar (Ø 21 – 353 mm) | SSAB specification; EN 10060 tolerances; EN 10308 ultrasonic testing |
| Hardness | EN ISO 6506-1 (Brinell) |
Tolerances and HS codes
- Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
- Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
- Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
| Form | NCM (Brazil, 8 digits) | HS (international, 6 digits) | HTS (USA, 10 digits)* | CN (European Union, 8 digits)* |
|---|---|---|---|---|
| Forged bar | 7228.40.00 | 7228.40 | 7228.40.0000 | 7228 40 90 |
| Hot-rolled bar | 7228.30.00 | 7228.30 | 7228.30.8041 | 7228 30 61 |
| Plate (> 10 mm, width ≥ 600 mm) | 7225.40.90 | 7225.40 | 7225.40.3050 | 7225 40 40 |
| Flange and fitting | 7307.91.00 | 7307.91 | 7307.91.5030 | 7307 91 00 |
Tariff class: alloy steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).
*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.
Chemical composition (%)
typical composition published by SSAB (606en); the value for each heat is on the certificate
| Element | Range (%) |
|---|---|
| C | 0.32 (typical) |
| Si | 0.9 (typical) |
| Mn | 0.8 (typical) |
| P | ≤ 0.011 |
| S | ≤ 0.003 |
| Cr | ≤ 1.70 |
| Ni | ≤ 1.4 |
| Mo | ≤ 1.40 |
| V | ≤ 0.17 |
Calculate the carbon equivalent of Toolox 44 – quenched and tempered tool steel for welding →
Mechanical properties
Quenched and tempered at a minimum of 590 °C (delivery condition); SSAB minimum values; rows marked "typical" are SSAB average values
| Property | Value |
|---|---|
| Hardness | 410 – 475 HBW (≈ 45 HRC nominal) |
| Yield strength Rp0.2 (plate 6 – 130 mm) | ≥ 1,150 MPa |
| Tensile strength (plate 6 – 130 mm) | ≥ 1,300 MPa |
| Elongation A5 (plate) | ≥ 8% |
| Round bar Ø 21 – 141 mm | Rp0.2 ≥ 1,100 MPa; Rm ≥ 1,250 MPa; A5 ≥ 8% |
| Charpy V at 20 °C | ≥ 18 J (plate, transverse; bar up to Ø 141 mm, longitudinal); ≥ 11 J (forged block and bar Ø 142 – 353 mm) |
| Typical hardness (plate) at 20 / 200 / 300 / 400 / 500 °C | 435 / 440 / 415 / 380 / 345 HBW (≈ 45 / 44 / 42 / 38 / 35 HRC) |
| Typical Rp0.2 (plate) at 20 / 200 / 300 / 400 / 500 °C | 1,300 / 1,150 / 1,040 / 980 / 825 MPa |
| Typical Rm (plate) at 20 / 200 / 300 / 400 / 500 °C | 1,405 / 1,340 / 1,270 / 1,190 / 1,010 MPa |
| Typical A5 (plate) at 20 / 200 / 300 / 400 / 500 °C | 13 / 10 / 12 / 14 / 19% |
| Typical Charpy V (plate) | 13 J at −20 °C; 30 J at 20 °C |
Typical physical properties
| Property | Value |
|---|---|
| Density | ≈ 7.85 g/cm³ (typical for alloy steel) |
| Thermal conductivity | 28 W/m·K at 20 °C; 30 at 200 °C; 29 at 400 °C (typical) |
| Thermal expansion | 11.0 / 12.5 / 14.2 × 10⁻⁶/K at 20 / 200 / 400 °C (typical) |
Calculate the weight of Toolox 44 – quenched and tempered tool steel bar, plate or pipe →
Heat treatment, welding and machining
| Item | Usual practice |
|---|---|
| Service temperature | Keeps its delivery hardness after being heated up to 590 °C, the minimum factory tempering temperature; above that, SSAB does not guarantee the properties. Used in hot forging dies working between 400 and 500 °C. |
| Heat treatment | Supplied quenched and tempered, with its final properties: no further treatment is needed. Heating above 590 °C voids the SSAB guarantees. Accepts nitriding (typically at 520 °C), laser or induction surface hardening and PVD coatings applied below 590 °C; under these conditions the core properties do not change. |
| Welding | Weldable and cuttable by thermal processes, with a low-hydrogen process and preheating according to thickness, following SSAB's welding recommendations for Toolox. Cold waterjet cutting is an alternative to thermal cutting. |
| Machining | Machined in the delivery condition with ordinary carbide tools. Since it is not quenched after machining and has low residual stress, the part does not distort or need corrective grinding. |
Plan an open-die forging in Toolox 44 – quenched and tempered tool steel: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →
Typical applications
- Plastic moulds
- Stamping and cutting dies
- Hot forging tools (continuous work at 400 – 500 °C)
- Highly stressed machine components
Alternatives: Toolox 33 and Toolox 40, from the same family, with lower hardness and more toughness, and Toolox 46, harder, for hot work; pre-hardened P20-type steels (1.2311 / 1.2738) and quenched and tempered 4140, with lower hardness; case by case, D2 (1.2379), as SSAB mentions. Conventional tool steels such as H13 (1.2344) need heat treatment after machining.
Frequently asked questions
What is the chemical composition of Toolox 44?
Per typical composition published by SSAB (606en); the value for each heat is on the certificate: C 0.32 (typical); Si 0.9 (typical); Mn 0.8 (typical); P ≤ 0.011; S ≤ 0.003; Cr ≤ 1.70.
Which standards cover Toolox 44?
Plate (6 – 130 mm): SSAB specification; EN 10029 tolerances (Toolox Thickness Guarantee); EN 10160 ultrasonic testing. Forged block (150 – 320 mm): SSAB specification; EN 10228-3 ultrasonic testing; flatness max. 1 mm/m. Round bar (Ø 21 – 353 mm): SSAB specification; EN 10060 tolerances; EN 10308 ultrasonic testing. Hardness: EN ISO 6506-1 (Brinell).
Up to what temperature can Toolox 44 be used?
Keeps its delivery hardness after being heated up to 590 °C, the minimum factory tempering temperature; above that, SSAB does not guarantee the properties. Used in hot forging dies working between 400 and 500 °C.
Which materials can replace Toolox 44?
Toolox 33 and Toolox 40, from the same family, with lower hardness and more toughness, and Toolox 46, harder, for hot work; pre-hardened P20-type steels (1.2311 / 1.2738) and quenched and tempered 4140, with lower hardness; case by case, D2 (1.2379), as SSAB mentions. Conventional tool steels such as H13 (1.2344) need heat treatment after machining.
Where to buy Toolox 44 in Brazil?
Dustre supplies Toolox 44 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to [email protected].