F51 vs F60: differences between S31803 and S32205
F51 and F60 are the same duplex 2205 in two composition ranges. F60 (UNS S32205) requires higher minimum chromium, molybdenum and nitrogen than F51 (S31803), which guarantees a higher minimum PREN, and it has a higher minimum tensile strength in ASTM A182. S32205 material also meets S31803, so most of it is sold dual certified F51/F60.
| Property | Duplex 2205 (F51 / S31803) | Duplex S32205 / F60 |
|---|---|---|
| Identification | ||
| Group | Duplex | Duplex |
| UNS | S31803 | S32205 |
| W.Nr. / EN | 1.4462 | 1.4462 |
| Chemical composition (%) | ||
| C | ≤ 0.030 | ≤ 0.030 |
| Mn | ≤ 2.00 | ≤ 2.00 |
| Si | ≤ 1.00 | ≤ 1.00 |
| P | ≤ 0.030 | ≤ 0.030 |
| S | ≤ 0.020 | ≤ 0.020 |
| Cr | 21.0–23.0 | 22.0–23.0 |
| Ni | 4.5–6.5 | 4.5–6.5 |
| Mo | 2.5–3.5 | 3.0–3.5 |
| N | 0.08–0.20 | 0.14–0.20 |
| Composition: standard | UNS S31803 (A240, A182 F51, A790) | UNS S32205 (A240, A182 F60, A790) |
| Mechanical properties (minimum) | ||
| Yield strength | – | – |
| Tensile strength | – | – |
| Elongation | – | – |
| Hardness | – | – |
| Properties: condition | A182 F51 (S31803), solution annealed | A182 F60 (S32205), solution annealed |
| Use and supply | ||
| PREN (minimum – typical) | 31 – 34 | 34 – 36 |
| Density | 7.8 g/cm³ | 7.8 g/cm³ |
| Service temperature | – | – |
| Standards by product form | Plate, coil, strip: A240 / SA-240 Bar and section: A276; A479 / SA-479 Forging and flange: A182 / SA-182 HIP part (powder metallurgy): A988 / SA-988 Seamless and welded pipe (piping): A790 / SA-790 | Plate, coil, strip: A240 / SA-240 Bar and section: A276; A479 / SA-479 Forging and flange: A182 / SA-182 HIP part (powder metallurgy): A988 / SA-988 Seamless and welded pipe (piping): A790 / SA-790 |
| Typical applications | Offshore oil and gas Chemicals and petrochemicals Pulp and paper Chemical tankers | Offshore oil and gas Chemicals and petrochemicals Pulp and paper Chemical tankers |
Composition and minimum properties per the standard listed on each datasheet; PREN uses the minimum and the middle of the ranges. For the actual value, use the heat certificate.
Most searched comparisons
- 316 / 316L stainless x 317L stainless steel
- Duplex 2205 (F51 / S31803) x Super duplex 2507 / F53 / S32750
- Inconel 625 / Alloy 625 x Incoloy 825
- 17-4PH stainless steel – UNS S17400 (ASTM A564 Type 630) x 15-5PH – UNS S15500 (XM-12)
- SAE 4140 x SAE 4340
For pitting resistance, see the PREN calculator; for steel weldability, the carbon equivalent; to choose by medium, steel by corrosive medium.
Frequently asked questions
Can F60 be used where F51 is specified?
Yes. The S32205 range fits inside the S31803 range, so an F60 heat meets F51. The opposite only holds if the heat also meets the S32205 minimums.
What is F51/F60 dual certification?
It is a certificate stating that the heat conforms to both designations, because its composition and properties meet both at the same time.
Which one should I ask for in a quote?
Ask for what the project requires. If the drawing says F51, an F51/F60 part works; if it says F60, the certificate must show S32205.