Materials comparator
Pick up to four materials and see side by side chemical composition, mechanical properties, PREN, service temperature, standards and applications. The data comes from the catalog datasheets.
| Property | 316 / 316L stainless | 317L stainless steel |
|---|---|---|
| Identification | ||
| Group | Stainless steels | Stainless steels |
| UNS | S31603 | S31703 |
| W.Nr. / EN | 1.4404 | ≈ 1.4438 (X2CrNiMo18-15-4) |
| Chemical composition (%) | ||
| C | ≤ 0.030 | ≤ 0.030 |
| Mn | ≤ 2.00 | ≤ 2.00 |
| Si | ≤ 0.75 | ≤ 1.00 (A240: ≤ 0.75) |
| P | ≤ 0.045 | ≤ 0.045 |
| S | ≤ 0.030 | ≤ 0.030 |
| Cr | 16.0–18.0 | 18.0 – 20.0 |
| Ni | 10.0–14.0 | 11.0 – 15.0 |
| Mo | 2.00–3.00 | 3.0 – 4.0 |
| N | ≤ 0.10 | ≤ 0.10 |
| Fe | – | balance |
| Composition: standard | ASTM A240 316L (S31603) | ASTM A182 F317L / A240 |
| Mechanical properties (minimum) | ||
| Yield strength | – | – |
| Tensile strength | – | – |
| Elongation | – | – |
| Hardness | – | – |
| Properties: condition | A182 F316L, solution annealed | Solution annealed (A182 F317L; A240 in parentheses) |
| Use and supply | ||
| PREN (minimum – typical) | 23 – 25 | 28 – 31 |
| Density | 7.98 g/cm³ | – |
| Service temperature | – | Oxidation acceptable up to ≈ 870 °C intermittent and ≈ 925 °C continuous. |
| Standards by product form | Plate, coil, strip: A240 / SA-240 Bar and section: A276 (general), A479 / SA-479 (pressure vessels) Forging and flange: A182 / SA-182; A336 (heavy forgings); A965 (high temperature) Seamless and welded pipe: A312 / SA-312; A358 (welded, large diameter); A376 (high temperature) Heat exchanger and boiler tube: A213 / SA-213 (seamless), A249 / SA-249 (welded), A269 (general), A270 (sanitary) | Bar: ASTM A276 Forging/flange: ASTM A182 F317L Plate: ASTM A240 Tube: ASTM A312 TP317L |
| Typical applications | Chemicals and petrochemicals Oil and gas and offshore Food, beverage and pharmaceutical Pulp and paper, water treatment | Flue gas desulfurization scrubbers (FGD) Pulp and paper (bleaching) Thermal power plant condensers Acetic, formic and dilute sulfuric acids |
Composition and minimum properties per the standard listed on each datasheet; PREN uses the minimum and the middle of the ranges. For the actual value, use the heat certificate.
Most searched comparisons
- 316 / 316L stainless x 317L stainless steel
- Duplex 2205 (F51 / S31803) x Super duplex 2507 / F53 / S32750
- Duplex 2205 (F51 / S31803) x Duplex S32205 / F60
- Inconel 625 / Alloy 625 x Incoloy 825
- 17-4PH stainless steel – UNS S17400 (ASTM A564 Type 630) x 15-5PH – UNS S15500 (XM-12)
- SAE 4140 x SAE 4340
For pitting resistance, see the PREN calculator; for steel weldability, the carbon equivalent; to choose by medium, steel by corrosive medium.
Frequently asked questions
How do I compare materials in the comparator?
Pick up to four materials from the catalog. The table shows side by side chemical composition, minimum mechanical properties, PREN, density, service temperature, standards by product form and applications, taken from each material's datasheet.
Are the values from the certificate?
No. They are the limits of the standard listed on each datasheet (composition and minimum properties). The actual heat values come on the quality certificate of the supplied material.
Can I share a comparison?
Yes. The page address stores the chosen materials after the # and opens the same comparison.