4140 vs 4340 steel: differences and when to use
4340 is a 4140 with about 1.8 % nickel. Nickel increases hardenability and toughness: quenched and tempered 4340 keeps core hardness in larger sections and resists impact better. 4140 (Cr-Mo) is cheaper and suits shafts, pins and gears of medium section.
| Property | SAE 4140 | SAE 4340 |
|---|---|---|
| Identification | ||
| Group | Carbon and alloy steels | Carbon and alloy steels |
| UNS | G41400 | G43400 |
| W.Nr. / EN | 42CrMo4 – 1.7225 (EN ISO 683-2) | ≈ 34CrNiMo6 – 1.6582 (EN ISO 683-2); ≈ 36CrNiMo4 – 1.6511 |
| Chemical composition (%) | ||
| C | 0.38 – 0.43 | 0.38 – 0.43 |
| Mn | 0.75 – 1.00 | 0.60 – 0.80 |
| Si | 0.15 – 0.35 | 0.15 – 0.35 |
| P | ≤ 0.035 | ≤ 0.035 |
| S | ≤ 0.040 | ≤ 0.040 |
| Cr | 0.80 – 1.10 | 0.70 – 0.90 |
| Ni | – | 1.65 – 2.00 |
| Mo | 0.15 – 0.25 | 0.20 – 0.30 |
| Fe | balance | balance |
| Composition: standard | SAE J404 / ASTM A29 | SAE J404 / ASTM A29 |
| Mechanical properties (minimum) | ||
| Yield strength | – | – |
| Tensile strength | – | – |
| Elongation | – | – |
| Hardness | – | – |
| Properties: condition | Quenched and tempered, section Ø 40–100 mm (EN 10083-3 / ISO 683-2, 42CrMo4 +QT); properties fall as the section increases | Quenched and tempered, section Ø 40–100 mm (reference 34CrNiMo6 +QT, EN 10083-3 / ISO 683-2) |
| Use and supply | ||
| PREN (minimum – typical) | – | – |
| Density | – | – |
| Service temperature | Up to ≈ 400–450 °C without relevant loss of properties (always below the tempering temperature). | Up to ≈ 400 °C in structural service, always below the tempering temperature. |
| Standards by product form | Bar (composition): SAE J404 / ASTM A29 / ABNT NBR NM 87 Quenched and tempered bar: ASTM A434 (classes BB, BC, BD) Forging: ASTM A668 / API 6A (75K) to customer specification Mechanical tubing: ASTM A519 Plate: ASTM A829 | Bar (composition): SAE J404 / ASTM A29 Quenched and tempered bar: ASTM A434 Aerospace bar/forging: AMS 6414 (VAR) / AMS 6415 Forging: ASTM A668 / to customer specification Mechanical tubing: ASTM A519 |
| Typical applications | Shafts, spindles and axle shafts Oil and gas forgings (bodies, bonnets, hangers – API 6A 75K) ASTM A193 B7 / B7M and A320 L7 studs and bolts (including for Petrobras) Quenched and tempered or nitrided gears and pinions | Large-section shafts and spindles Heavy transmission gears and crown wheels Landing gear and aircraft structural components (VAR) Highly stressed crankshafts and connecting rods |
Composition and minimum properties per the standard listed on each datasheet; PREN uses the minimum and the middle of the ranges. For the actual value, use the heat certificate.
Most searched comparisons
- 316 / 316L stainless x 317L stainless steel
- Duplex 2205 (F51 / S31803) x Super duplex 2507 / F53 / S32750
- Duplex 2205 (F51 / S31803) x Duplex S32205 / F60
- Inconel 625 / Alloy 625 x Incoloy 825
- 17-4PH stainless steel – UNS S17400 (ASTM A564 Type 630) x 15-5PH – UNS S15500 (XM-12)
For pitting resistance, see the PREN calculator; for steel weldability, the carbon equivalent; to choose by medium, steel by corrosive medium.
Frequently asked questions
Which one for a large shaft?
For large diameters, with core hardness or impact requirements, 4340. For medium sections, 4140 usually does the job.
Do both weld well?
Both need preheating and hydrogen control; 4340, with a higher carbon equivalent, needs more care. See the carbon equivalent calculator.
Can I replace 4140 with 4340?
Yes, 4340 works wherever 4140 works. Adjust tempering to the hardness specified on the drawing.