316L vs 317L: differences and when to use each
317L is a reinforced 316L: more chromium (18–20 % vs 16–18 %) and more molybdenum (3–4 % vs 2–3 %). This raises the PREN and the resistance to pitting and acids, which is why 317L is used in flue gas scrubbers (FGD), pulp bleaching and condensers. For water, food and mild chemicals, 316L is enough and easier to find in every product form.
| Property | 316 / 316L stainless | 317L stainless steel |
|---|---|---|
| Identification | ||
| Group | Stainless steels | Stainless steels |
| UNS | S31603 | S31703 |
| W.Nr. / EN | 1.4404 | ≈ 1.4438 (X2CrNiMo18-15-4) |
| Chemical composition (%) | ||
| C | ≤ 0.030 | ≤ 0.030 |
| Mn | ≤ 2.00 | ≤ 2.00 |
| Si | ≤ 0.75 | ≤ 1.00 (A240: ≤ 0.75) |
| P | ≤ 0.045 | ≤ 0.045 |
| S | ≤ 0.030 | ≤ 0.030 |
| Cr | 16.0–18.0 | 18.0 – 20.0 |
| Ni | 10.0–14.0 | 11.0 – 15.0 |
| Mo | 2.00–3.00 | 3.0 – 4.0 |
| N | ≤ 0.10 | ≤ 0.10 |
| Fe | – | balance |
| Composition: standard | ASTM A240 316L (S31603) | ASTM A182 F317L / A240 |
| Mechanical properties (minimum) | ||
| Yield strength | – | – |
| Tensile strength | – | – |
| Elongation | – | – |
| Hardness | – | – |
| Properties: condition | A182 F316L, solution annealed | Solution annealed (A182 F317L; A240 in parentheses) |
| Use and supply | ||
| PREN (minimum – typical) | 23 – 25 | 28 – 31 |
| Density | 7.98 g/cm³ | – |
| Service temperature | – | Oxidation acceptable up to ≈ 870 °C intermittent and ≈ 925 °C continuous. |
| Standards by product form | Plate, coil, strip: A240 / SA-240 Bar and section: A276 (general), A479 / SA-479 (pressure vessels) Forging and flange: A182 / SA-182; A336 (heavy forgings); A965 (high temperature) Seamless and welded pipe: A312 / SA-312; A358 (welded, large diameter); A376 (high temperature) Heat exchanger and boiler tube: A213 / SA-213 (seamless), A249 / SA-249 (welded), A269 (general), A270 (sanitary) | Bar: ASTM A276 Forging/flange: ASTM A182 F317L Plate: ASTM A240 Tube: ASTM A312 TP317L |
| Typical applications | Chemicals and petrochemicals Oil and gas and offshore Food, beverage and pharmaceutical Pulp and paper, water treatment | Flue gas desulfurization scrubbers (FGD) Pulp and paper (bleaching) Thermal power plant condensers Acetic, formic and dilute sulfuric acids |
Composition and minimum properties per the standard listed on each datasheet; PREN uses the minimum and the middle of the ranges. For the actual value, use the heat certificate.
Most searched comparisons
- Duplex 2205 (F51 / S31803) x Super duplex 2507 / F53 / S32750
- Duplex 2205 (F51 / S31803) x Duplex S32205 / F60
- Inconel 625 / Alloy 625 x Incoloy 825
- 17-4PH stainless steel – UNS S17400 (ASTM A564 Type 630) x 15-5PH – UNS S15500 (XM-12)
- SAE 4140 x SAE 4340
For pitting resistance, see the PREN calculator; for steel weldability, the carbon equivalent; to choose by medium, steel by corrosive medium.
Frequently asked questions
Can 317L replace 316L?
Yes, in corrosion resistance 317L works wherever 316L works. The switch is only not worth it when 316L already resists the medium, because 317L is less common in stock and costs more.
Do the mechanical properties change?
Very little. Both are low-carbon, solution-annealed austenitic grades with very similar minimum values. The choice between them is driven by corrosion.
Which one is easier to weld?
Both weld well. On 317L, a filler metal with more molybdenum (such as ER317L or a nickel alloy) is used so the weld is not less resistant than the plate.