Alloy 59 – UNS N06059
Very-low-carbon nickel-chromium-molybdenum alloy, tungsten-free
Ni-Cr-Mo alloy with about 23% Cr and 16% Mo, carbon up to 0.010% and iron up to 1.5%. It resists oxidizing and reducing media, pitting and crevice corrosion in chlorides, and stress corrosion cracking. It is one of the C-family alloys with the highest overall resistance and keeps the weld zone resistant without post-weld treatment.
Designations and equivalents
| System | Designation |
|---|---|
| UNS | N06059 |
| W.Nr./EN | 2.4605 – NiCr23Mo16Al |
| DIN | NiCr23Mo16Al |
| Trade names | Alloy 59; manufacturers' trade names (e.g. VDM Alloy 59, Nicrofer 5923 hMo) are trademarks of those manufacturers |
Standards by product form
| Form | Standard |
|---|---|
| Bar | ASTM B574 |
| Forging | ASTM B564 |
| Plate | ASTM B575 |
| Tube | ASTM B622 (seamless), B619 and B626 (welded) |
| Fittings | ASTM B366 |
| Filler metal | AWS A5.14 ERNiCrMo-13 |
Tolerances and HS codes
- Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
- Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
- Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
| Form | NCM (Brazil, 8 digits) | HS (international, 6 digits) | HTS (USA, 10 digits)* | CN (European Union, 8 digits)* |
|---|---|---|---|---|
| Forged bar | 7505.12.10 | 7505.12 | 7505.12.3000 | 7505 12 00 |
| Hot-rolled bar | 7505.12.10 | 7505.12 | 7505.12.3000 | 7505 12 00 |
| Plate (> 10 mm, width ≥ 600 mm) | 7506.20.00 | 7506.20 | 7506.20.3000 | 7506 20 00 |
| Seamless pipe | 7507.12.00 | 7507.12 | 7507.12.0000 | 7507 12 00 |
| Welded pipe | 7507.12.00 | 7507.12 | 7507.12.0000 | 7507 12 00 |
| Flange and fitting | 7507.20.00 | 7507.20 | 7507.20.0000 | 7507 20 00 |
Tariff class: nickel alloy (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).
*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.
Chemical composition (%)
ASTM B574 (UNS N06059)
| Element | Range (%) |
|---|---|
| Ni | balance |
| Cr | 22.0 – 24.0 |
| Mo | 15.0 – 16.5 |
| Fe | ≤ 1.5 |
| Al | 0.1 – 0.4 |
| Co | ≤ 0.3 |
| Mn | ≤ 0.5 |
| Si | ≤ 0.10 |
| C | ≤ 0.010 |
| P | ≤ 0.015 |
| S | ≤ 0.010 |
Mechanical properties
solution annealed (ASTM B574 / B564)
| Property | Value |
|---|---|
| Yield strength (0.2%) | ≥ 310 MPa |
| Tensile strength | ≥ 690 MPa |
| Elongation | ≥ 45% |
Typical physical properties
| Property | Value |
|---|---|
| Density | 8.6 g/cm³ |
| Melting range | 1,310 – 1,360 °C* |
| Modulus of elasticity | 210 GPa* |
| Thermal conductivity (20 °C) | 10.4 W/m·K* |
| Thermal expansion (20–100 °C) | 11.9 µm/m·K* |
Heat treatment, welding and machining
| Item | Usual practice |
|---|---|
| Service temperature | An alloy for aqueous corrosion, from cryogenic up to about 425 °C in the ASME allowable stress tables (II-D)*. Avoid prolonged exposure between 600 and 1,000 °C, the range of intermetallic phase precipitation. |
| Heat treatment | Solution annealing between 1,100 and 1,180 °C* with rapid cooling (water or forced air). Not age hardenable. |
| Welding | Good weldability, with no preheating or post-weld treatment. Filler metals: AWS A5.14 ERNiCrMo-13 (TIG and MIG) and AWS A5.11 ENiCrMo-13 (covered electrode). Low heat input and interpass up to 150 °C. |
| Machining | Difficult: it work hardens quickly; use carbide, low speed, constant feed without stopping on the part, and abundant coolant. |
Plan an open-die forging in Alloy 59: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →
Typical applications
- Reactors and heat exchangers in the chemical industry
- Flue gas desulfurization (FGD) and scrubbers
- Bleaching in pulp and paper
- Pharmaceuticals and fine chemicals
- Effluent treatment and incineration
- Components in seawater and hot brines
- Weld overlay cladding
Alternatives: Hastelloy C-276 and C-22 in much the same media; Inconel 625 in moderate media, at lower cost; Hastelloy B-2 in hot concentrated hydrochloric acid.
Compare alloys by corrosive medium, concentration and temperature →
Alloy 59: complete guide
What Alloy 59 is
Alloy 59 (UNS N06059, W.Nr. 2.4605) is a nickel alloy of the nickel-chromium-molybdenum group, the same as C-276 and C-22. It has more chromium than C-276 (22.0–24.0% versus 14.5–16.5%) and practically the same molybdenum (15.0–16.5% versus 15.0–17.0%), contains no tungsten, and limits carbon to 0.010% and iron to 1.5%, which reduces precipitation in the weld heat-affected zone.
Chemical composition and the role of the elements
Chromium (22 to 24%) protects in oxidizing media; molybdenum (15 to 16.5%) protects in reducing media and against pitting and crevice corrosion; aluminum (0.1 to 0.4%) is added as a deoxidizer. By the Cr + 3.3 Mo formula, the PREN is around 75, among the highest in the family.
Mechanical properties
Solution annealed, ASTM B574 requires a minimum yield strength of 310 MPa, a minimum tensile strength of 690 MPa and a minimum elongation of 45%. The alloy is not heat-treatable; strength only increases by cold work.
Corrosion and limits of use
It resists dilute sulfuric and hydrochloric acids, acids with chlorides, wet chlorine, hypochlorites, seawater and hot brines, including media that alternate between oxidizing and reducing. To choose between 59 and other alloys in your medium, use the steel by corrosive medium calculator and the PREN calculator.
Supply forms and Dustre services
Bars and blocks forged in open die, cut to size on a band saw, with machining, solution annealing in our own furnaces and hardness, tensile and impact testing. Material with a 3.1 inspection certificate and heat traceability.
Frequently asked questions
What is the chemical composition of Alloy 59?
Per ASTM B574 (UNS N06059): Ni balance; Cr 22.0 – 24.0; Mo 15.0 – 16.5; Fe ≤ 1.5; Al 0.1 – 0.4; Co ≤ 0.3.
Which standards cover Alloy 59?
Bar: ASTM B574. Forging: ASTM B564. Plate: ASTM B575. Tube: ASTM B622 (seamless), B619 and B626 (welded). Fittings: ASTM B366. Filler metal: AWS A5.14 ERNiCrMo-13.
Up to what temperature can Alloy 59 be used?
An alloy for aqueous corrosion, from cryogenic up to about 425 °C in the ASME allowable stress tables (II-D)*. Avoid prolonged exposure between 600 and 1,000 °C, the range of intermetallic phase precipitation.
Which materials can replace Alloy 59?
Hastelloy C-276 and C-22 in much the same media; Inconel 625 in moderate media, at lower cost; Hastelloy B-2 in hot concentrated hydrochloric acid.
Where to buy Alloy 59 in Brazil?
Dustre supplies Alloy 59 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to [email protected].